A mould review is not a beauty contest for the 3D model. It is five drawings: gate location, ejection layout, cooling circuit, venting, and slides or lifters. If any one of them is missing, the problem it would have caught waits until the T0 trial - and at that point you are cutting steel, not editing a drawing.
The gate drawing decides three things at once, which is why it takes up most of the review time: where the weld lines land, which way the part will warp, and whether packing pressure can reach the far end of the cavity. A proper gate sheet shows the injection points and their type, the runner dimensions, and a prediction of weld-line positions. Hold it against the appearance drawing and ask the obvious question: does a weld line land on a glossy or light-transmitting face? If it does, move the gate. On paper that is one dot relocated; after the tool is cut it is a core insert remade.
Ejection is an appearance issue, cooling is a cycle-time issue. On ejection, check two things: whether pins land on weak faces, and whether the total push area is enough. A pin on a thin wall or on a rib leaves a white mark, sometimes a puncture; the practical rule is to keep pins against ribs and boss positions, where the stiffness is highest. On cooling, uniformity matters more than presence. Water too far from the cavity face runs slow and lengthens the cycle; too close and you get local overcooling that pulls stress marks out of the part. The usual check figure is 1.5 to 2 times the water hole diameter from centre to cavity face, and that number should be verified line by line during the review. Deep pockets and thick sections deserve a separate look, because that is where the steel is still soft at demould and the part deforms under the ejector - they often need a baffle or a beryllium-copper insert.
The three most frequently missing drawings are venting, slides and lifters, and venting carries the highest price for its small size. On many mould drawings it is one line: provide vents per standard practice. But vent positions are calculated: the last place the melt reaches, the points where flow fronts meet, and the bottom of deep pockets all require venting. Vent depth sits in the 0.02 to 0.03 mm band - deeper and the melt flees into it and leaves flash, shallower and it does nothing. Get it wrong and the symptom is a corner that scorches repeatedly at trial, and every correction means remachining an insert. Slides and lifters must be drawn separately to check stroke, interference and spring return; these do not show up as problems in a 3D model. We have seen a slide short of stroke by 2 mm tear an undercut white - measurable on paper before any steel moved.
Two practical points. A review of all five drawings properly takes two to three hours, mostly on gate and ejection; a half-hour sign-off means the sheets were not read. And when a mould shop answers with standard practice, ask instead for a process note attached at quotation stage: gate type, ejection method, water layout, vent positions. It costs nothing to provide and it filters out the shops that never really looked at the part.