Acrylic is PMMA. Three numbers decide whether a clear housing works: 92% light transmittance, 0.3% water absorption, and 1.5-2 kJ/m² notched impact strength. The first two make it beautiful and easy to mould. The third is why it cracks when it hits the floor.
Only one of the three can be moved by structural design. Transmittance sits around 92% for standard grades; absorption near 0.3%, which is why pellets must be dried at 80°C for four hours before moulding - above 0.05% residual moisture you get silver streaks. Impact strength is 1.5-2 kJ/m², roughly a tenth of polycarbonate. That brittleness belongs to the material, not to a bad batch.
Two structural remedies exist. Keep walls at 2mm or thicker, and keep inside corner radii at least as large as the wall. We built a 1.5mm clear panel that shattered at the corners in a one-metre drop test; the same geometry at 2.2mm passed. On PMMA, the corner matters more than the wall. Our drawing standard sets inner radius at exactly one wall thickness, outer radius at half the sum of both walls, so nobody guesses 0.3 or 0.5 by feel.
Yellowing is usually diagnosed in the wrong order. Cut the part and look at the section: a yellow layer 0.2-0.3mm deep on the lit face is UV ageing; yellow spreading radially from the gate is moulding stress; a hazy, silver-streaked part throughout is under-dried resin. Only when both features point at the material should you suspect the compound. Reverse that order and you will change a batch of resin for nothing.
Ribs should never sit on a light-transmitting face. Read through the part and the sink mark at the rib root shows as a white shadow that paint cannot hide. If you need stiffness, thicken the frame or move the rib to the back of an opaque border.
Use PMMA for display windows, lamp covers, panels and light guides: dimensionally stable, hard, resists wiping scratches, and holds its appearance longer than PC. Switch away from it for load-bearing parts, snap fits that are opened repeatedly, and anything left outdoors. Bearing parts belong in polycarbonate, with ten times the impact strength; outdoor parts need UV-stabilised tinted resin or PC with a hard coat. One question settles it: will this part be dropped, or will it sit in the sun for two years?
Above roughly 300-500 pieces, injection moulding beats cut-and-bond sheet; below that, cutting, bonding and heat bending win because you skip tooling. Complex curves, internal snaps and ribs cannot be cut at all.